01 Fabricator removes: welding slag, paint, heavy grease, Avoid silicone/oil based anti-spatter sprays
02 Degrease: removes light oil/grease alkaline or acidic solution
03 Rinse
04 Chemical clean: hydrochloric acid, ambient temperature, removes rust and mill scale
05 Rinse
06 Flux: 30% zinc ammonium chloride solution, 65℃-85℃, aids wetting of steel by molten zinc, sometimes flux blanket
07 Dry: not always necessary, useful for tubular work
08 Galvanize: min. 98.5% zinc, 450℃, typical 5-20 minutes immersion
09 Quench: optional, cool the work, apply post-treatments